10' - 14' Random Lengths
A.S.T.M. A276 (except 303)
Continental Steel will cut to any length you desire. With our precision high-speed equipment, we can give prompt attention to large and small cut piece requirements.
Specifications
Material |
N/A Type 304 Stainless Steel |
Shapeform |
N/A Hexagon Bar |
Size |
N/A 1 1/16 inches |
Size |
N/A 1.0625 inches26.9875 mm |
Weight |
N/A 3.3247 lbs/ft4.9471536 kg/m |
Weight per 12' Length |
N/A 39.897 lbs18.073341 kg |
Finish |
N/A No. 2B |
Condition |
N/A Cold Drawn Annealed |
Nominal Composition |
N/A 0 to 0.25% Carbon 1.00% Max. Silicon 2.00% Max. Manganese 6 to 36% Nickel 7 to 30% Chrome |
ASTM Specification |
N/A ASTM A276 UNS S30400 |
Random Length |
N/A 10 to 14 ft |
Typical Mechanical Properties
Steel Alloy Group |
N/A Austenitic |
Magnetic Properties |
N/A Non-Magnetic |
Harden By |
N/A Cold Work |
Corrosion Resistance |
N/A High |
Hardness |
N/A Low to Med. |
Strength |
N/A Low to Med. |
Ductility |
N/A High |
Toughness |
N/A High |
Elec. Conductance |
N/A Low |
Thermal Conductance |
N/A Low |
Thermal Expansion |
N/A High |
Heat Resistance (Scaling Strength) |
N/A High/High |
Comparative Characteristics and Applications
Yield Strength |
N/A 46000 lbs/in² |
Tensile Strength |
N/A 89000 lbs/in² |
Elongation percent in 2 inches |
N/A 55 % |
Hardness (Rockwell B) |
N/A 86 |
Creep Strength Load for 10000 Hr. with 1% Elongation at 1000°F |
N/A 17000 lbs/in² |
Creep Strength Load for 10000 Hr. with 1% Elongation at 1100°F |
N/A 12000 lbs/in² |
Creep Strength Load for 10000 Hr. with 1% Elongation at 1200°F |
N/A 7000 lbs/in² |
Creep Strength Load for 10000 Hr. with 1% Elongation at 1300°F |
N/A 4000 lbs/in² |
Density |
N/A 0.29 lbs/in³ |
Modulus of Elasticity in Tension |
N/A 28.0 x 106 lbs/in² |
Specific Heat (32 to 212°F) |
N/A 0.12 BTU/ºF/lbs |
Thermal Conductivity at 212°F |
N/A 9.4 BTU/hr.ft²/ft/ºF |
Thermal Conductivity at 932°F |
N/A 12.4 BTU/hr.ft²/ft/ºF |
Mean Coefficient of Thermal Expansion per °F (32 to 212°F) |
N/A 9.6 x 10-6 ºF |
Mean Coefficient of Thermal Expansion per °F (32 to 600°F) |
N/A 9.9 x 10-6 ºF |
Mean Coefficient of Thermal Expansion per °F (32 to 1000°F) |
N/A 10.2 x 10-6 ºF |
Mean Coefficient of Thermal Expansion per °F (32 to 1200°F) |
N/A 10.4 x 10-6 ºF |
Melting Point Range |
N/A 2550 to 2650 ºF |
Electrical Resistivity |
N/A 72 µΩ.cm |
Max. Operating Temp. (Continuous Service) |
N/A 1650 ºF |
Max. Operating Temp. (Intermittent Service) |
N/A 1500 ºF |
Welding Properties |
N/A Very Good-Tough Welds |
Drawing and Stamping |
N/A Very Good |
Hot Working - Initial Forging |
N/A 2100 to 2300 ºF |
Annealing Temp. |
N/A 1850 to 2050 ºF |
Stress Relieving Temp. |
N/A 400 to 750 ºF |
Applications
N/A
|